Analysis of plate corrosion and rubber mat aging in plate heat exchanger

Plate heat exchanger as a compact and efficient heat exchange equipment, although its development has been nearly a hundred years old, and in some sectors (such as food, pharmaceutical, chlor-alkali, etc. Industry) has a wide range of applications, but due to its lack of temperature, pressure, corrosion resistance and other capabilities, it limits its application. In the evaporation section of the ion membrane workshop of a factory in our company, two MB100 plate heat exchangers are used to cool the lye in parallel. The hot fluid inlet medium of the heat exchanger is an alkali solution (containing a small amount of salt) with a temperature above 85 °C, and is exported. The temperature is about 50 °C. The plate heat exchanger is made of 304 stainless steel plate, which suppresses the adult-shaped 0.6mm thick corrugated plate, and is composed of a labyrinth-shaped fluid passage with a reversed left and right herringbone groove. After two years of use, the plate heat exchanger leaked, and the plate heat exchanger was prevented from leaking after one month. The following is a brief analysis of the reasons for the failure of the plate heat exchanger.
Sealing failure
Seam gasket material
The detachable plate heat exchanger leaks when used, and the failure of the gasket material is an important factor in addition to sheet corrosion. There are mainly the following ways: 1 When the rubber gasket material is in contact with the fluid, when a fluid component penetrates into the rubber, sometimes the soluble substance can be extracted, resulting in swelling of the rubber gasket; 2 the presence of halogen and ozone The effect is to soften the gasket or cause stress corrosion cracking. 3 Under certain conditions, especially at high temperatures, the elastic material will decompose and release chemicals, which themselves will corrode the sheet material, such as FPM rubber will release oxygen. After disassembling the plate heat exchanger, it was found that the cold fluid end surface of the plate was bright, a small amount of black scale was locally, the number of corrosion pits was small and did not penetrate, and there was black deposit in the corrosion pit, so it can be inferred as a gasket. Piece of corrosion exists.
Fluid pressure
Removable plate heat exchangers leak when used within the rated working pressure, except for the quality factors in the manufacturing assembly, mainly in the system The water hammer and the air hammer are related to the abnormal impact load, which is a phenomenon that is not easily observed during use. The instantaneous pressure peak caused by the impact is often 1-3 times higher than the normal working pressure, causing the rubber gasket installed in the plate heat exchanger to shift, resulting in seal failure. Since the heat transfer element of the device is made of a stainless steel sheet (thickness of 0.5-1.0 mm), the sealing rigidity is relatively poor and the sealing perimeter is long, so the impact pressure resistance is much lower than that of the shell-and-tube heat exchanger. The abnormal impact of the plate heat exchanger can be judged according to the equipment for providing the conveying medium. When the alkali pump for transporting the alkali liquid to the plate heat exchanger is repaired, it is found that there is a small amount of honeycomb in the pump casing, indicating that the pump is running. There is cavitation; at the same time, due to the leakage around the previous plate, it can be inferred that the change of fluid pressure is also a possible factor of leakage.
Temperature
A sharp change in temperature can also cause seal failure. When the temperature changes too fast, the coefficient of linear expansion of the rubber gasket does not match the elastic deformation amount and the sealing pre-tightening force, so that the sealing pre-tightening force is lowered, and the pressure bearing capacity of the device is lower than the rated design pressure.
From the working conditions of the plate heat exchanger, the temperature has little effect on it, so it can be excluded.
Corrosion
The corrosion of plate heat exchangers mainly refers to the corrosion of the plates. Plate heat exchangers are mostly made of stainless steel sheets. Although stainless steel has good corrosion resistance, it will cause uniform or partial corrosion of the stainless steel sheets after the passivation film is destroyed. The corrosion phenomenon exhibited by the plate heat exchanger is mostly stress corrosion caused by Cl-, which often occurs at the bottom of the sealing groove of the plate and the bottom of the scale after the formation of dirt. The main reason is that: 1 stainless steel plate is mechanically cold pressed. Inevitably, a certain amount of surface residual stress remains inevitably. For a stainless steel sheet containing no molybdenum element, the elimination of surface residual stress is difficult. After the two sheets are assembled, a multi-slit structure is formed, and the corrugated top ends of the adjacent sheets cross each other to form a large number of contacts. There will be gaps in the cross-contacts, and the medium in the gaps will not flow smoothly, so that there is a difference in the concentration of oxygen inside and outside the gap, causing crevice corrosion. 3 When the dirt on the surface of the plate is serious, the corrosion elements (Cl, S, etc.) in the medium may adhere to the dirt in a large amount and be enriched in the gap of the bottom. 4 The harmful elements in the bottom of the sealing groove are often the precipitation of Cl in the adhesive due to temperature rise. For example, the neoprene series of adhesives and compressed asbestos mats (containing CaCl2) tend to form ClCl and H+ in the water and steam conditions, resulting in severe stress corrosion at the bottom of the groove. Cracking. When the unpacked sheets were inspected, it was found that most of the sheets at the inlet of the hot fluid side had cracks, and there was a thick layer of dark brown deposit before the cleaning; on the hot-fluid inlet side of the sheet, the top of the herringbone corrugated, adjacent The contacts on the top of the corrugated corrugations have point-like surface damage and corrosion spots, surrounded by dark brown deposits. Perforation corrosion occurs in 1 or 2 places on each plate, and is located at the cross-over contacts of the corrugated tip near the hot fluid inlet side, and the local area is corroded pitting and pit. The crack on the side of the hot fluid in the perforated corrosion pit is obvious, and most of the corrosion is in the shape of a slit, and most of it has penetrated. Therefore, it can be judged that the corrosion condition of the plate heat exchanger is a comprehensive reaction of various factors.
Analysis and Discussion
According to the above analysis and test results, the heat exchanger plate failure is mainly corrosion failure,
The heat exchanger uses EPDM as a gasket. Due to the high inlet temperature and the pressing force, the S element in the pad is in contact with the plate. Produces a certain sulfide that promotes the occurrence and expansion of corrosion.
The heat exchanger is composed of a plurality of plates alternately arranged and pressed together, and the corrugated top ends of adjacent plates cross each other to form a large number of contacts. There will be gaps on the cross-contacts, and the medium in the gaps will not flow or flow poorly, resulting in a difference in the concentration of oxygen inside and outside the gap, causing crevice corrosion, causing certain areas in the gap to preferentially corrode and dissolve, which is in contact The main cause of perforation corrosion at the point.
contains a small amount of sodium chloride in the lye, so that the plate contains a higher concentration of Cl- ions in the gap, due to its strong penetrating ability, damage It even penetrates the surface passivation film, so that the base metal directly contacts the medium, causing corrosion to dissolve; the presence of the S element may generate some sulfide, which promotes the occurrence and expansion of corrosion.
The heat exchanger herringbone corrugated sheet is stamped and formed into a large amount of martensite, and the crystal is dispersed into fine carbides. Stainless steel has reduced corrosion resistance. The residual stress after deformation, together with the tightening force applied during the assembly of the sheet, causes large stresses at the top of the corrugation, promotes intergranular corrosion, and causes cracks to propagate along the crystal.
In the operating system, when the heat exchanger is subjected to an abnormal impact exceeding the rated load, the displacement of the gasket is liable to occur and leakage is caused.
The quality and service life of plate heat exchangers depends to a large extent on the quality and service life of the gasket. For large logarithmic heat exchangers, the plates are generally not damaged, and the gaskets are prone to aging and cause leakage, so the quality of the gasket determines the quality and service life of the heat exchanger.  
2019/05/11 08:34:07 6002 Click

欧美性VIDEOS高清精品| 天天躁日日躁很很很躁| 成熟丰满熟妇自慰XXXXX| 午夜精品久久久久久久| 久久夜色精品国产噜噜亚洲AV| 差差差无掩盖视频30分钟| 亚洲AV成人无码影视网| 欧美精产国品一二三产品区别| 国产青草视频在线观看| 777成了乱人视频| 午夜无码伦费影视在线观看果冻| 欧美成本人网站免费观看| 国产探花在线精品一区二区| AAA日本高清在线播放免费观看| 亚洲AV激情无码专区在线播放| 欧美猛少妇色XXXXX猛叫| 国产亚洲欧美精品一区| JAPANESE成熟丰满熟妇| 亚洲精品WWW久久久久久| 日韩久久无码免费毛片软件| 久久无码高潮喷水免费看| 国产成人AV无码精品| 67194熟妇在线直接进入百度| 亚洲 欧洲 小说 自拍| 人妻少妇精品视频无码综合 | 97久久天天综合色天天综合色H | 色老头精品午夜福利视频| 久久无码人妻精品一区二区三区 | 免费无码又爽又刺激高潮软件| 国产亚洲成AV人片在线观看导航 | 波多野结衣HD在线观看 | 新版АⅤ资源新版在线天堂| 欧洲免费无码视频在线| 久久久亚洲精品无码| 国精产品999国精产品官网| 动性配人ⅩXXXX配| 99无码人妻一区二区三区免费| 亚洲熟妇无码八AV在线播放| 性XXXX欧美老妇506070| 色五月五月丁香亚洲综合网| 欧美人妻少妇精品久久黑人| 领导在办公室含我奶头口述| 精品浪潮av一区二区三区| 国产精品V片在线观看不卡| 被青梅竹马的学弟给锁定了林擎霄 | 天堂AV亚洲ITV在线AⅤ| 欧美最猛激情性AAAAA| 麻豆亚洲AV成人无码久久精品| 激情久久AV一区AV二区AV三| 国产精品国产三级国产AV′| 成人国产精品一区二区网站公司| 8Ⅹ8X擦拨擦拨成人免费视频 | 国产亚洲精品美女久久久久| 国产92成人精品视频免费| YYY6080韩国三级理论| 18禁黄网站禁片免费观看国产| 亚洲影院丰满少妇中文字幕无码| 亚洲成A人片77777国产| 午夜A级毛片免费观看| 私はあなたのおさんです怎么读| 日本亚洲色欲网站WWW| 欧美人妻少妇精品久久黑人| 你的奶好大让老子摸摸的说说| 麻豆乱码国产一区二区三区| 久久久久久久无码高潮| 精品乱码一卡2卡三卡4卡二卡| 国产亚洲精品自在久久VR| 国产精品青青在线麻豆| 国产成人精品久久久久| 公交车后车座疯狂的做的细节| 成人无码视频免费播放| 成人毛片100免费观看| 啊轻点灬大JI巴太粗太长了在线| FREEXX性黑人大战欧美| AV天堂影音先锋AV色资源网站| 99久久精品免费看国产| AA区一区二区三无码精片| av 成人 亚洲无码| chinese人妻无码人妻| 99麻豆久久久国产精品免费 | 2021国产手机在线精品| 中日大胆裸体棚拍人体| 中文字幕人成无码人妻综合社区| 中文字幕人妻无码一夲道| 2021精品久久久久精品免费网| 99精品人妻少妇一区二区| APPSTORE美区免费| А√ 天堂 在线官网中文| 波多野结衣的影片| 疯狂做受XXXX国产| 国产精品国产三级国产专I| 国产日韩未满十八禁止观看| 韩国无码AV片在线观看网站| 极品YIN荡人妻合集H| 精品无码成人片一区二区| 久久亚洲精品无码GV| 男人J进女人屁网站免费| 欧美一级 片内射欧美乱强 | 里番ACG ※里番_ACG工口| 蜜桃女同一区二区免费AV哟| 欧美黑人又大又粗XXXX| 日韩精品成人无码专区免费| 四川50岁熟妇大白屁股真爽| 香蕉久久AⅤ一区二区三区| 亚洲卡5卡6卡7卡2021入口| 野草高清视频免费| 7M精品福利视频导航| 拔萝卜影视剧免费观看| 国产SUV精品一区二区88L| 国产午夜成人无码免费看不卡| 久久99精品久久久久久9| 免费AV资源网站| 日本人XXXX裸体XXXX| 无码成人黄动漫在线观看| 亚洲国产精品无码第一区二区三区 | 亚洲国产精品久久一线APP| 永久免费精品精品永久-夜色| 99精品国产一区二区三区2| 草莓丝瓜向日葵黄瓜榴莲IOS| 国产成人亚洲精品无码高潮 | 国产7色在线 | 国产| 国产亚洲精品拍拍拍拍拍| 久久久久久精品免费无码无| 女人爽到高潮的免费视频| 日韩A片无码ⅩXXXX| 性开放按摩AV大片| 夜夜夜高潮夜夜爽夜夜爰爰| WWW国产亚洲精品久久麻豆| 国产精品扒开腿做爽爽爽日本无码| 娇妻借朋友高H繁交H| 男女爽到高潮的免费网站| 色偷偷亚洲第一成人综合网址| 亚洲AV激情高潮抽搐乱色| 永久免费的AV在线网无码| 草莓视频APP无限观看| 国产综合在线观看| 免费毛片45分钟| 天堂√最新版中文在线天堂| 亚洲色在线无码国产精品不卡| JAPANESE国产永久| 国产品无码一区二区三区在线蜜桃 | 关灯后在线高清免费观看| 激情综合丁香五月| 欧美高潮抽搐喷水大叫| 玩弄丰满少妇人妻视频| 一本久道综合在线无码88| 宝宝两根就哭男男是不是太早了| 国产人无码A在线西瓜影音| 乱肉怀孕又粗又大| 色悠久久久久综合欧美99| 亚洲精品午夜久久久伊人| А√天堂中文官网在线地址| 国语对白露脸XXXXXX| 欧美成人精品三级网站视频| 西西午夜无码大胆啪啪国模| 18一20亚洲GAY无套| 国产精品爽爽VA在线观看无码| 么公的好大好硬好深好爽视频 | 民工把我奶头掏出来了怎么办| 国产精品无码不卡一区二区三区| 久久丫精品国产亚洲AV| 色窝窝人妻9色聚色窝| 亚洲一区二区三区国产精华液| 成人用品有限公司| 久久99精品久久水蜜桃| 日出水了特别黄的视频| 亚洲中文字幕无码人在线| 干了快生了的孕妇| 乱精品一区字幕二区| 无码人妻精品一区二区蜜桃天美| 综合图区亚洲欧美另类图片| 国产熟女一区二区| 人妻夜夜添夜夜无码AV| 亚洲色成人一区二区三区小说| 妇女性内射冈站HDWWW000| 蜜桃视频在线观看| 亚洲AV不卡无码国产| 把腿张开老子臊烂你的黄漫| 九九久久亚洲AV东方伊甸园| 少妇毛又多又黑一区二区| 中文在线っと好きだった官网 | 锕锕锕锕锕锕~好深啊APP| 国产中年熟女高潮大集合| 日本三级韩国三级欧美三级| 一本一本久久A久久综合精品| 国产精品99久久免费观看| 欧亚激情偷乱人伦小说专区| 亚洲一线产区二线产区区别在哪里 | 天天躁夜夜躁天干天干2020| 99国内精品久久久久久久漫画 | 国产午夜福利短视频在线观看| 人人做人人爽人人爱| 在线|国产精品女主播阳台| 国语自产第1国语自产第10页| 日日噜噜夜夜狠狠久久蜜桃 | 丰满人妻被公侵犯完整版| 欧美变态口味重另类在线视频| 亚洲香蕉一本大道在线| 国产偷自视频区视频| 少妇一晚三次一区二区三区|